2022-01-13
1170
|
奥氏体不锈钢 | UNS牌号:S30400 | 通用材料牌号:304 | |||||||||||||||||
序号 | 类别 | 材料牌号 | 引用标准 | 化学成分 | 机械性能 | |||||||||||||||
C | Mn | P | S | Si | Ni | Cr | N | Cu | 其它 |
屈服 强度σ0.2 |
拉伸 强度 |
延伸率 (纵向) |
硬度 |
断面 收缩率 |
热处理/ Quench Media |
|||||
% | % | % | % | % | % | % | % | % | % | % | (MPa) | (MPa) | % | HBW | (%) | ℃/冷却 | ||||
1 | 美标管件 | WP304 | ASTM A403/403M-20 | ≤0.08 | ≤2.00 | ≤0.045 | ≤0.030 | ≤1.00 | 8.00-11.00 | 18.00-20.00 | ≥205 | ≥515 | ≥28 | ≥1040℃/水冷 | ||||||
2 | 美标钢管 | TP304 | ASTM A312/312M-21 | ≤0.08 | ≤2.00 | ≤0.045 | ≤0.030 | ≤1.00 | 8.00-11.00 | 18.00-20.00 | ≥205 | ≥515 | ≥35 | 1040℃/水冷 | ||||||
3 | 美标板材 | 304 | ASTM A240/A240M-20 | ≤0.07 | ≤2.00 | ≤0.045 | ≤0.030 | ≤0.75 | 8.00-10.50 | 17.5-19.5 | ≤0.10 | ≥205 | ≥515 | ≥40 | ≤201 | |||||
4 | 美标锻件 | F304 | ASTM A182/182M-21 | ≤0.08 | ≤2.00 | ≤0.045 | ≤0.030 | ≤1.00 | 8.00-11.00 | 18.00-20.00 | ≤0.10 | ≥205 | ≥515 | ≥30 | ≥50 | 1040℃/水冷 | ||||
5 | 国标管件 | SF304 | GB/T13401-2017 | ≤0.08 | ≤2.00 | ≤0.045 | ≤0.030 | ≤1.00 | 8.00-11.00 | 17.50-20.00 | ≥205 | ≥515 | ≥30 | ≤201 | 固溶处理 | |||||
6 | 国标钢管 |
06Cr19Ni10 (S30408) |
GB/T14976-2012 | ≤0.08 | ≤2.00 | ≤0.035 | ≤0.030 | ≤1.00 | 8.00-11.00 | 18.00-20.00 | ≥205 | ≥520 | ≥35 | 1010-1150℃ /水冷 | ||||||
7 | 国标锻件 |
06Cr19Ni10 (S30408) |
NB/T47010-2017 | ≤0.08 | ≤2.00 | ≤0.035 | ≤0.015 | ≤1.00 | 8.00-11.00 | 18.00-20.00 | ≥220 |
≥520 ≥500 |
≥35 |
139-192 131-192 |
1010-1150℃ /水冷 | |||||
8 | 欧标管件 | 1.4301 | EN10253-4:2008 | ≤0.07 | ≤2.00 | ≤0.045 | ≤0.015 | ≤1.00 | 8.00-10.50 | 17.00-19.50 | ≤0.11 |
σ0.2≥195 σ1.0≥230 |
500-700 | ≥40 | ≤200 |
at-196℃ ≥60 |
1000-1100℃ /水冷 | |||
9 | 欧标锻件 | 1.4301 | EN10222-5:2017 | ≤0.07 | ≤2.00 | ≤0.045 | ≤0.015 | ≤1.00 | 8.0-10.5 | 17.5-19.5 | ≤0.10 |
σ0.2≥200 σ1.0≥230 |
500-700 | ≥45 |
at-196℃ ≥60 |
1000-1100℃/水冷 |